Specify 6061-T6 for most machined aluminum parts: it is strong enough, machines cleanly, welds, and anodizes well at a moderate price. Choose 7075-T6 when you need roughly 80 percent more strength and will not weld it. Choose 5052-H32 for sheet metal that gets bent, welded, or lives near salt water.
How do 6061, 7075, and 5052 compare?
The values below are typical published properties for each alloy in its common temper. Actual mill certificates vary slightly by product form and thickness, so use these for comparison, not for final design.
| Property (typical) | 6061-T6 | 7075-T6 | 5052-H32 |
|---|---|---|---|
| Ultimate tensile strength | 45 ksi (310 MPa) | 83 ksi (572 MPa) | 33 ksi (228 MPa) |
| Yield strength | 40 ksi (276 MPa) | 73 ksi (503 MPa) | 28 ksi (193 MPa) |
| Elongation | about 12% | about 11% | about 12% |
| Brinell hardness | 95 | 150 | 60 |
| Elastic modulus | 10.0 Msi (69 GPa) | 10.4 Msi (72 GPa) | 10.2 Msi (70 GPa) |
| Density | 0.098 lb/in3 | 0.102 lb/in3 | 0.097 lb/in3 |
| Heat treatable | Yes | Yes | No (strain hardened) |
| Arc weldability | Good | Poor | Excellent |
| Machinability | Good | Good to excellent | Fair |
| Corrosion resistance | Good | Fair | Excellent |
When should I use 6061?
6061-T6 is the default for good reason. It is a magnesium and silicon alloy that machines with a clean chip, holds a good surface finish, welds with common filler wires, and takes a clear or colored anodize well. It is widely stocked as plate, bar, tube, and extrusion, which keeps material cost and lead time down.
Use 6061 for brackets, housings, fixtures, plates, manifolds, enclosures, and most general mechanical parts. If you are not sure which aluminum to call out, 6061-T6 is rarely the wrong answer.
One thing to know: welding 6061-T6 reduces the strength near the weld significantly, because the heat undoes the T6 temper in that zone. Welded 6061 structures should be designed to the as-welded strength, or the assembly re-heat-treated after welding.
When is 7075 worth the extra cost?
7075 is a zinc alloy and one of the strongest common aluminum alloys. In T6 temper its yield strength is higher than that of common structural mild steel such as A36, at about one third the weight. It machines very well, often better than 6061, with small chips and a bright finish.
Use 7075 for highly loaded parts where weight matters: arms, levers, structural fittings, mounts that see shock loads, and tooling that takes abuse.
The trade-offs:
- It is not considered weldable by ordinary arc processes. It cracks, and the weld zone loses strength. Bolt or pin it.
- Corrosion resistance is lower than 6061 or 5052. In T6 temper it can be susceptible to stress corrosion cracking under sustained tensile stress. The T73 temper trades some strength for much better resistance, and is worth asking about for parts under constant load in a wet environment.
- It costs more per pound than 6061 and is stocked in fewer sizes.
- It is not stiffer. This is the most common misunderstanding. If a 6061 part bends too much, switching to 7075 will not fix it. Only geometry does.
When should I choose 5052?
5052 is a magnesium alloy that gets its strength from cold working rather than heat treatment. The H32 temper is the common sheet temper. It bends to tight radii without cracking, welds very well, and has the best salt-water corrosion resistance of the three.
Use 5052 for sheet metal enclosures, panels, covers, fuel and water tanks, boat parts, and anything that is formed and welded. It is less suited to heavily machined parts: it is softer, the chip tends to be stringy, and it is mostly sold as sheet and thin plate rather than bar.
A practical rule: if the part starts as a flat pattern and gets bent, think 5052. If it starts as a block and gets machined, think 6061 or 7075.
How does each alloy anodize?
All three anodize, with differences in appearance:
- 6061 gives a consistent, clear finish and takes dye colors evenly. It is the common choice for cosmetic anodized parts.
- 7075 anodizes well for protection and hardcoat, though the zinc content can give a clear anodize a slightly different tone than 6061. If parts from both alloys sit side by side, expect a visible difference.
- 5052 anodizes well and gives a bright, clean clear finish.
If color match matters across an assembly, specify the same alloy for every visible part. Anodizing also changes dimensions slightly, so call out which features must be measured after finishing.
Which aluminum is cheapest to machine?
Total cost is material plus machine time. 6061 usually wins overall: the material is the least expensive of the three in most forms, and it machines quickly. 7075 machines just as fast or faster, but the material costs more. 5052 bar is less common and the material is slower to cut cleanly, so it is rarely the cheapest choice for a machined block even when the material itself is inexpensive.
How should I call out aluminum on a drawing?
Give the alloy and the temper, and the specification if your industry requires one:
- "6061-T6" or "6061-T651" for plate (the 51 means stress relieved by stretching, which helps flatness after machining)
- "7075-T651" for plate parts that need strength
- "5052-H32" for sheet
Avoid "aluminum" with no alloy. It leaves the choice to the shop and can lead to a part that does not match the next batch.
Getting the part made
Culmination Machine Works machines 6061, 7075, and 2024 aluminum along with steels, stainless, titanium, and plastics. For a grade not on that list, ask when you request a quote. See the materials guide and 3 and 5 axis CNC machining, or send your drawing with the alloy you have in mind and we will tell you if another one suits the part better.
Frequently asked questions
No. Both have an elastic modulus of roughly 10 million psi (about 69 to 72 GPa). 7075 is much stronger, so it can take more load before it yields, but under the same load a 7075 part bends almost exactly as much as a 6061 part of the same shape. To reduce deflection, add material or change the shape.
It is generally treated as not weldable by ordinary arc welding because it is prone to hot cracking, and any weld loses most of the T6 strength. Design 7075 parts to be bolted or pinned. If the part must be welded, use 6061 or 5052.
5052 is a softer, non-heat-treatable alloy. It tends to form long, gummy chips and build up on the cutting edge, which makes a clean finish harder to hold. It is excellent for sheet metal parts that are bent and welded, and less ideal for heavily machined blocks.
5052 has the best salt-water corrosion resistance of the three, and 6061 is also widely used in marine hardware. 7075 has lower corrosion resistance and should be protected with a coating or anodize if it lives near salt water.